保温材料
泡沫混凝土应用技术规程JGJ/T 341-2014
泡沫混凝土 | |||||
检验项目 | 技术指标 | 价格 | |||
干密度(kg/m3) | 密度等级 | 干密度pd(kg/m3) | 200 | ||
标准值 | 允许范围 | ||||
A01 | 100 | 50<pd ≤150 | |||
A02 | 200 | 150<pd ≤250 | |||
A03 | 300 | 250<pd ≤350 | |||
A04 | 400 | 350<pd ≤450 | |||
A05 | 500 | 450<pd ≤550 | |||
A06 | 600 | 550<pd ≤650 | |||
A07 | 700 | 650<pd ≤750 | |||
A08 | 800 | 750<pd ≤850 | |||
A09 | 900 | 850<pd ≤950 | |||
A10 | 1000 | 950<pd ≤1050 | |||
A11 | 1100 | 1050<pd ≤1150 | |||
A12 | 1200 | 1150<pd ≤1250 | |||
A13 | 1300 | 1250<pd ≤1350 | |||
A14 | 1400 | 1350<pd ≤1450 | |||
A15 | 1500 | 1450<pd ≤1550 | |||
A16 | 1600 | 1550<pd ≤1650 | |||
抗压强度(MPa) | 强度等级 | 抗压强度(MPa) | 300 | ||
每组平均值 | 每块最小值 | ||||
FC0.2 | 0.20 | 0.170 | |||
FC0.3 | 0.30 | 0.255 | |||
FC0.5 | 0.50 | 0.425 | |||
FC1 | 1.00 | 0.850 | |||
FC2 | 2.00 | 1.700 | |||
FC3 | 3.00 | 2.550 | |||
FC4 | 4.00 | 3.400 | |||
FC5 | 5.00 | 4.250 | |||
FC7.5 | 7.50 | 6.375 | |||
FC10 | 10.00 | 8.500 | |||
FC15 | 15.00 | 12.760 | |||
FC20 | 20.00 | 17.000 | |||
FC25 | 25.00 | 21.250 | |||
FC30 | 30.00 | 25.500 | |||
导热系数 | 密度等级 | 导热系数[W/(m·K)] | 400 | ||
A01 | ≤0.05 | ||||
A02 | ≤0.06 | ||||
A03 | ≤0.08 | ||||
A04 | ≤0.10 | ||||
A05 | ≤0.12 | ||||
A06 | ≤0.14 | ||||
A07 | ≤0.18 | ||||
A08 | ≤0.21 | ||||
A09 | ≤0.24 | ||||
A10 | ≤0.27 | ||||
A11 | ≤0.29 | ||||
A12 | ≤0.31 | ||||
A13 | ≤0.33 | ||||
A14 | ≤0.37 | ||||
A15 | ≤0.41 | ||||
A16 | ≤0.46 | ||||
注:表中导热系数由泡沫混凝土含水率为6%时测定,自然状态下可乘以1.25的修正系数。 | |||||
抗冻性 | 使用条件 | 抗冻标号 | - | ||
非采暖地区 | D15 | 1000 | |||
采暖地区 | 相对湿度≤60% | D25 | 1000 | ||
相对湿度>60% | D35 | 1400 | |||
干湿交替部位和水位变化部位 | ≥D50 | 2200 +1次+40元 | |||
注:1.非采暖地区系指最冷月份的平均气温高于-5℃的地区; 2.采暖地区系指最冷月份的平均气温低于或等于-5℃的地区; 3.保温泡沫混凝土以保温系统抗冻性试验进行检测。 | |||||
现浇泡沫混凝土(硬化泡沫混凝土性能) | |||||
检验项目 | 技术指标 | 价格 | |||
干密度(kg/m3) | 密度等级 | 干密度pd(kg/m3) | 200 | ||
标准值 | 允许范围 | ||||
A01 | 100 | 50<pd ≤150 | |||
A02 | 200 | 150<pd ≤250 | |||
A03 | 300 | 250<pd ≤350 | |||
A04 | 400 | 350<pd ≤450 | |||
A05 | 500 | 450<pd ≤550 | |||
A06 | 600 | 550<pd ≤650 | |||
A07 | 700 | 650<pd ≤750 | |||
A08 | 800 | 750<pd ≤850 | |||
A09 | 900 | 850<pd ≤950 | |||
A10 | 1000 | 950<pd ≤1050 | |||
A11 | 1100 | 1050<pd ≤1150 | |||
A12 | 1200 | 1150<pd ≤1250 | |||
A13 | 1300 | 1250<pd ≤1350 | |||
A14 | 1400 | 1350<pd ≤1450 | |||
A15 | 1500 | 1450<pd ≤1550 | |||
A16 | 1600 | 1550<pd ≤1650 | |||
抗压强度(MPa) | 强度等级 | 抗压强度(MPa) | 300 | ||
每组平均值 | 每块最小值 | ||||
FC0.2 | 0.20 | 0.170 | |||
FC0.3 | 0.30 | 0.255 | |||
FC0.5 | 0.50 | 0.425 | |||
FC1 | 1.00 | 0.850 | |||
FC2 | 2.00 | 1.700 | |||
FC3 | 3.00 | 2.550 | |||
FC4 | 4.00 | 3.400 | |||
FC5 | 5.00 | 4.250 | |||
FC7.5 | 7.50 | 6.375 | |||
FC10 | 10.00 | 8.500 | |||
FC15 | 15.00 | 12.760 | |||
FC20 | 20.00 | 17.000 | |||
FC25 | 25.00 | 21.250 | |||
FC30 | 30.00 | 25.500 | |||
导热系数 | 密度等级 | 导热系数[W/(m·K)] | 400 | ||
A01 | ≤0.05 | ||||
A02 | ≤0.06 | ||||
A03 | ≤0.08 | ||||
A04 | ≤0.10 | ||||
A05 | ≤0.12 | ||||
A06 | ≤0.14 | ||||
A07 | ≤0.18 | ||||
A08 | ≤0.21 | ||||
A09 | ≤0.24 | ||||
A10 | ≤0.27 | ||||
A11 | ≤0.29 | ||||
A12 | ≤0.31 | ||||
A13 | ≤0.33 | ||||
A14 | ≤0.37 | ||||
A15 | ≤0.41 | ||||
A16 | ≤0.46 | ||||
注:表中导热系数由泡沫混凝土含水率为6%时测定,自然状态下可乘以1.25的修正系数。 | |||||
抗冻性 | 使用条件 | 抗冻标号 | - | ||
非采暖地区 | D15 | 1000 | |||
采暖地区 | 相对湿度≤60% | D25 | 1000 | ||
相对湿度>60% | D35 | 1400 | |||
干湿交替部位和水位变化部位 | ≥D50 | 2200 +1次+40元 | |||
注:1.非采暖地区系指最冷月份的平均气温高于-5℃的地区; 2.采暖地区系指最冷月份的平均气温低于或等于-5℃的地区; 3.保温泡沫混凝土以保温系统抗冻性试验进行检测。 | |||||
干燥收缩值mm/m 适用于密度等级为A07~A16的泡沫混凝土 | ≤1 | 400 | |||
吸水率,% | 应符合现行行业标准《泡沫混凝土》JG/T266的规定 | 500 | |||
线膨胀系数,1/℃ | 8×10-6 | 另议 | |||
燃烧性能 | A1级 | 1500 | |||
建筑构件的耐火极限 | 应符合现行国家标准《建筑设计防火规范》GB50016的规定。 | 6000/首h +0.5h+1000 | |||
泡沫混凝土保温板的性能 | |||
检验项目 | 技术指标 | 价格 | |
Ⅰ型 | Ⅱ型 | ||
干密度,kg/m3 | ≤180 | ≤250 | 100 |
抗压强度,MPa | ≥0.30 | ≥0.40 | 200 |
导热系数(平均温度25℃±2℃),W/(m·K) | ≤0.055 | ≤0.065 | 400 |
干燥收缩值(浸水24h),mm/m | ≤3.5 | ≤3.0 | 400 |
垂直于板面的抗拉强度kPa | ≥80 | ≥100 | 200 |
燃烧性能 | A1级 | 1500 | |
软化系数 | ≥0.70 | 400 | |
体积吸水率,% | ≤10 | 500 | |
碳化系数 | ≥0.70 | 500 | |
放射性 | 同时满足内照射指数IR≤1.0 和外照射指数Iy≤1.0 | 1000 | |